Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with 15HC blade recommend for thermal spray coatings | ||||
Mounting | Castable, typically with epoxy drawn under vacuum | ||||
Apex DGD Red | 75 µm diamond water cooled | 5 [22] | 300 |
![]() |
Until Plane |
Apex Hercules S Rigid Grinding Disc | 9 µm MetaDi Supreme Diamond | 5 [22] | 150 |
![]() |
4:00 |
TriDent | 3 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
3:00 |
ChemoMet | 0.02 -0.06 µm MasterMet or MasterMet 2 Colloidal Silica | 6 [27] | 150 |
![]() |
2:00 |