Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Sectioning Precision Saw with 20LC blade recommended for hard tough materials
Mounting Castable, typically epoxy with added flat -edge filler
Apex Hercules H Rigid Grinding Disc 30 µm MetDi Supreme Diamond 6 [27] 150 -200 Rotation Image Until Plane
Apex Hercules S Rigid Grinding Disc 9 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 4:00
VerduTex 3 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 3:00
ChemoMet 0.02 -0.06 µm MasterMet or MasterMet 2 Colloidal Silica 6 [27] 150 Rotation Image 2:00