Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with a blade recommended for use on soft gummer materials | ||||
Mounting | Castable, typically with EpoThin 2 | ||||
CarbiMet | 240 [P280] grit SiC water cooled | moderate | 400 |
![]() |
Until Plane |
CarbiMet | 320 [P400] grit SiC water cooled | moderate | 400 |
![]() |
1:00 |
CarbiMet | 400 [P800] grit SiC water cooled | moderate | 400 |
![]() |
1:00 |
CarbiMet | 600 [P1200] grit SiC water cooled | moderate | 400 |
![]() |
1:00 |
TriDent | 6 µm Metadi Supreme Diamond | moderate | 400 |
![]() |
2:00 |
MasterTex | 1 µm MetaDi Supreme Diamond | moderate | 400 |
![]() |
2:00 |