Sectioning | Precision Saw with 30HC blade recommnded for polymers | ||||
Mounting | Castable, typically EpoThin 2 | ||||
Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
CarbiMet | 320 [P400] grit SiC water cooled | 4 [18] | 300 |
![]() |
Until Plane |
CarbiMet | 400 [P800] grit SiC water cooled | 4 [18] | 300 |
![]() |
1:00 |
CarbiMet | 600 [P1200] grit SiC water cooled | 4 [18] | 300 |
![]() |
1:00 |
CarbiMet | 1200 [P2500] grit SiC water cooled | 4 [18] | 300 |
![]() |
1:00 |
TexMet C | 3 µm MetaDi Supreme Diamond | 5 [22] | 150 |
![]() |
4:00 |
MasterTex | 0.05 µm MasterPrep Alumina | 3 [13] | 150 |
![]() |
3:00 |