SumMet method for NI -BASED SUPERALLYS
Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Sectioning Abrasive Cutter with a wheel recommended for use on SuperAlloys
Mounting Compression, typically with EpoMet
CarbiMet 240 [P280] grit SiC water cooled 6 [27] 300 Rotation Image Until Plane
Apex Hercules S Rigid Grinding Disc 9 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 5:00
TriDent 3 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 5:00
ChemoMet 0.02 -0.06 µm MasterMet or MasterMet 2 Colloidal Silica 6 [27] 150 Rotation Image 2:00