Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Abrasive Cutter with a wheel recommended for use on SuperAlloys | ||||
Mounting | Compression, typically with EpoMet | ||||
CarbiMet | 240 [P280] grit SiC water cooled | 6 [27] | 300 |
![]() |
Until Plane |
UltraPad | 9 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
5:00 |
TriDent | 3 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
3:00 |
TriDent | 1 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
2:00 |
ChemoMet | 0.02 -0.06 µm MasterMet or MasterMet 2 Colloidal Silica | 6 [27] | 150 |
![]() |
2:00 |