Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with 15LC blade recommended for hard brittle materials | ||||
Mounting | Castable, typically EpoThin 2 or EpoHeat 2 | ||||
Apex DGD | 45 µm diamond water cooled | 5 [22] | 300 |
![]() |
3:00 |
TriDent | 9 µm MetaDi Supreme Diamond | 3 [13] | 150 |
![]() |
4:00 |
TriDent | 3 µm MetaDi Supreme Diamond | 3 [13] | 150 |
![]() |
4:00 |
TexMet C | 0.05 µm MasterPrep Alumina | 4 [18] | 150 |
![]() |
2:00 |