Scroll to Top
  1-847-295-6500 Call Buehler at 1-847-295-6500 Search Buehler

SumMet method for IRON - ALTERNATE METHOD

SumMet method for IRON - ALTERNATE METHOD
Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Sectioning Abrasive Cutter with a wheel recommended for use on ferrous materials HRC35 -60
Mounting Compression or Castable, typically with EpoMet or VariDur 3000
Apex DGD Red 75 µm Diamond water cooled 6 [27] 300 Rotation Image Until Plane
Apex Hercules S Rigid Grinding Disc 9 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 5:00
TriDent 3 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 3:00
MicroCloth 0.05 µm MasterPrep Alumina 6 [27] 150 Rotation Image 2:00