Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with 15LC blade recommended for hard brittle materials | ||||
Mounting | Castable, typically EpoThin 2 or EpoHeat 2 | ||||
CarbiMet | 320 [P400] grit SiC water cooled | 5 [22] | 300 |
![]() |
Until Plane |
CarbiMet | 400 [P800] grit SiC water cooled | 5 [22] | 300 |
![]() |
1:00 |
TexMet P | MiroMet (CeO) 1 µm | 5 [22] | 150 |
![]() |
5:00 |
MicroCloth | MiroMet (CeO) 1 µm | 5 [22] | 150 |
![]() |
2:00 |