Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with 15LC blade recommended for glass | ||||
Mounting | Castable | ||||
Apex DGD | 45 µm diamond water cooled | 5 [22] | 300 |
![]() |
5:00 |
Apex DGD | 15 µm diamond water cooled | 5 [22] | 300 |
![]() |
5:00 |
Apex DGD | 3 µm diamond water cooled | 5 [22] | 300 |
![]() |
5:00 |
TexMet C | 3 µm MetaDi Supreme Diamond | 5 [22] | 150 |
![]() |
4:00 |
MasterTex | MasterPolish 2 | 5 [22] | 150 |
![]() |
4:00 |