Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Precision Saw with 10LC or 20LC blade recommended for medium to soft ceramics or structural ceramics | ||||
Mounting | Castable, typically epoxy with flat edge filler if for very hard ceramic applications | ||||
Apex DGD Red | 75 µm diamond water cooled | 8 [36] | 300 |
![]() |
Until Plane |
TexMet P | 15 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
6:00 |
VerduTex | 6 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
4:00 |
VerduTex | 3 µm MetaDi Supreme Diamond | 6 [27] | 150 |
![]() |
4:00 |