Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Sectioning Precision Saw with 15HC blade recommended for metal matrix composites
Mounting Castable, typically epoxy
UltraPrep Metal -Bonded Disc 45 µm diamond water cooled 6 [27] 300 Rotation Image Until Plane
UltraPad 15 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 4:00
VerduTex 6 µm MetaDi Supreme Diamond 6 [27] 150 Rotation Image 3:00
VerduTex 1 µm MetaDi Supreme Diamond 150 Rotation Image 2:00