Scroll to Top
  1-847-295-6500 Call Buehler at 1-847-295-6500 Search Buehler

SumMet method for CAST IRON

SumMet method for CAST IRON
Surface Abrasive / Size Load - lbs [N] / Specimen Base Speed [rpm] Relative Rotation Time [min:sec]
Sectioning Abrasive cutter with a wheel recommended for use on ferrous materials HRC35 -50
Mounting Compression or Castable
CarbiMet 320 [P400] grit SiC water cooled 5 [22] 300 Rotation Image Until Plane
TexMet C 9 µm MetaDi Supreme Diamond 5 [22] 150 Rotation Image 5:00
TriDent 3 µm MetaDi Supreme Diamond 5 [22] 150 Rotation Image 4:00
MicroCloth 0.05 µm MasterPrep Alumina 5 [22] 150 Rotation Image 2:00