Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Abrasive Cutter with a wheel recommended for use on non -ferrous materials | ||||
Mounting | Compression or Castable, typically with PhenoCure, EpoxiCure 2, EpoThin 2 or SamplKwick | ||||
CarbiMet | 320 [P400] grit SiC water cooled | 5 [22] | 300 |
![]() |
Until Plane |
UltraPad | 9 µm MetaDi Supreme Diamond | 5 [22] | 150 |
![]() |
5:00 |
TriDent | 3 µm MetaDi Supreme Diamond | 5 [22] | 150 |
![]() |
4:00 |
ChemoMet | 0.06 µm MasterMet Colloidal Silica | 5 [22] | 150 |
![]() |
1:30 |