Surface | Abrasive / Size | Load - lbs [N] / Specimen | Base Speed [rpm] | Relative Rotation | Time [min:sec] |
---|---|---|---|---|---|
Sectioning | Abrasive Cutter with a wheel recommended for use on ferrous materials HRC35 -50 | ||||
Mounting | Compression, typically with EpoMet | ||||
CarbiMet | 120 [P120] to 320 grit [P400] SiC water cooled | 6 [27] | 300 | Until Plane | |
UltraPad | 9 µm MetaDi Supreme Diamond* | 6 [27] | 150 | 5:00 | |
TriDent | 3 µm MetaDi Supreme Diamond* | 6 [27] | 150 | 3:00 | |
ChemoMet | 0.05 µm MasterPrep Alumina | 6 [27] | 150 | 2:00 |